Laboratory Electrical Resistivity Studies on Cement Stabilized Soil

Table 1

Compaction and strength characteristics of the soil cement samples.

ParameterSoil-cement samples
A0A2A4A6B0B2B4B6C0C2C4C6D0D2D4D6

, kN/m3 (LC)14.514.614.814.615.615.615.015.415.915.715.615.616.416.616.716.6
OMC (%) (LC)28.028.326.825.625.022.425.22423.222.823.423.221.020.618.820.4
, (kN/m3) (HC)14.916.416.416.515.917.317.317.716.418.318.418.217.518.818.418.4
OMC (%) (HC)27.022.121.921.622.019.019.017.221.014.41616.518.014.915.416
7-day UCS (kPa) (LC)130.8478.8814.8991.7155.6733863.61691.8162.2769.31307.31703.5289.21080.81507.52130.2
C (kPa) (LC)23.5290.0340.0480.021.0265.0280.0390.019.0190.0245.0320.018.5140.0180.0260.0
(degrees) (LC)20.031.035.040.025.034.036.041.031.037.041.043.031.038.046.051.0
STS (kPa) (LC)75.52109.9112.864.1104.2107.0352.6101.3104.255.598.4101.3

Note. : max dry density, OMC: optimum moisture content, LC: light compaction, HC: heavy compaction, UCS: unconfined compressive strength, C: cohesion, : angle of internal friction, and STS: split tensile strength.