Characterization and Beneficiation of an Egyptian Nepheline Syenite Ore
Table 8
Magnetic separation followed by reverse anionic flotation.
| Separation step | Product | Product Wt., % | Assay | Distribution | Fe2O3, % | Al2O3, % | Fe2O3, % | Al2O3, % |
| Magnetic Sep. Step (−0.125 mm feed size) | Magnetic | 23.7 | 25.1 | 8.1 | 93.7 | 11.64 | Nonmag. | 76.3 | 0.52 | 21.1 | 6.3 | 88.36 | Total | 100 | 6.49 | 18.1 | 100 | 100 |
| Flotation Step (−0.074 mm feed size) | Froth | 20.5 (15.6)* | 1.8 | 10.2 | 69.9 (4.33)* | 9.9 (8.2)* | Bulk | 79.5 (60.7)* | 0.2 | 23.9 | 30.1 (1.86)* | 90.2 (80.2)* | Total | 100 (76.3)* | 0.53 | 21.1 | 100 (6.3)* | 100 (88.4)* |
|
|
Values in parentheses are calculated based on the head sample.
|