Research Article
T4 and T6 Treatment of 6061 Al-15 Vol. % SiCP Composite
Table 3
The Brinell hardness values of T6-treated 6061 Al-SiC composite.
| Time of aging (hours) | Brinell hardness (In MPa) of the composite aged at | 140°C | 160°C | 180°C | 200°C | 220°C | 240°C |
| 0 | 893.7 | 893.7 | 893.7 | 893.7 | 893.7 | 893.7 | 0.5 | 1097.6 | 1166.2 | 1244.6 | 1234.8 | 1205.4 | 1195.6 | 1 | 1156.4 | 1225 | 1313.2 | 1332.8 | 1283.8 | 1254.4 | 2 | 1195.6 | 1293.6 | 1401.4 | 1372 | 1362.2* | 1274* | 3 | 1215.2 | 1313.2 | 1430.8 | 1401.4* | 1332.8 | 1254.4 | 4 | 1244.6 | 1323 | 1450.4* | 1342.6 | 1313.2 | 1244.6 | 5 | 1264.2 | 1352.4* | 1401.4 | 1323 | 1283.8 | 1215.2 | 6 | 1274* | 1313.2 | 1352.4 | 1264.2 | 1234.8 | 1195.6 | 8 | 1254.4 | 1225 | 1303.4 | 1205.4 | 1205.4 | 1185.8 | 10 | 1234.8 | 1185.8 | 1244.6 | 1185.8 | 1185.8 | 1176 | 20 | 1117.2 | 1136.8 | 1146.6 | 1127 | 1136.8 | 1127 |
|
|
*Peak hardness.
|