Research Article

Steam Reforming of Glycerol for Hydrogen Production over Catalyst

Table 1

Physical characteristics of Ni/SiO2 catalysts.

Catalyst - (size-mm)No. of hours/cyclesNi crystallite size (nm) form XRDSurface composition from EDAXCarbon (%) from CHNS analysisBET surface area (m2/g)
Ni %C %

NS - (2 × 2) 5.057 260
NS1 - (2 × 2)68 h5.76.37760107
NS2 - (2 × 4)20 h6.8402525150
NS3 - (3 × 5)100 h7.8252020125
NS4 - (3 × 5)20 cy12.5283530145
NS5 - (3 × 5)20 cy*20.137.61215

Number of hours of the run = h; number of cycles operated = cy.
GWMRs: 1 : 9 *GWMRs: 1 : 18.
NS = Ni/SiO2 (fresh catalyst); NS1, NS2, NS3, NS4, and NS5 = Ni/SiO2 (used catalysts).