Mortar mixes proportions.

IndexCement
Kg/m3
Silica fume
Kg/m3
Water
Kg/m3
Sp.
Kg/m3
Sand
Kg/m3
W/Bpalm fiber volumetric fraction %Flow
mm

M05504024011.814150.430140
M15504024011.814150.430.2130
M25504024011.814150.430.4125
M35454024011.814050.430.6125
M45454024011.814050.430.8120
M55404024011.813900.431.0115
M65404024011.813900.431.2120
M75354024011.813800.431.4115
M85354024011.813800.431.6110