Research Article
Bitumen Coating as a Tool for Improving the Porosity and Chemical Stability of Simulated Cement-Waste Forms
Table 5
The compressive strength values of coated and non-coated cemented blocks at different periods of immersion in various media.
| Immersion time, (days) | Compressive strength (MPa) | Tapwater | Groundwater | Seawater | Non-coated | Coated | Non-coated | Coated | Non-coated | Coated |
| 0 | 44.79 | 21.4 | 44.79 | 21.4 | 44.79 | 21.4 | 30 | 31 | 18.7 | 29.0 | 23.3 | 27.4 | 18.6 | 60 | 32.5 | 27.7 | 30.8 | 25.1 | 30.87 | 23.05 | 90 | 35.4 | 28.8 | 32.8 | 26.2 | 33.1 | 24.8 |
|
|