Research Article
Fracture Surface Analysis in Thixojoined Tool Steels
Table 1
Microstructural data as a function of holding time and temperature of AISI D2 steel.
| Temp. (°C) | Holding time (min.) | Liquid fraction (%fl) | Shape factor (SF) | Ave. Grains size (m) |
| 1280 | 5 | 12 | 0.8 | 35 | 10 | 15 | 0.85 | 50 | 15 | 17 | 0.8 | 55 | 20 | 18 | 0.78 | 65 |
| 1300 | 5 | 15 | 0.86 | 40 | 10 | 18 | 0.85 | 45 | 15 | 25 | 0.78 | 50 | 20 | 26 | 0.75 | 55 |
| 1320 | 5 | 25 | 0.74 | 50 | 10 | 30 | 0.7 | 50 | 15 | 36 | 0.68 | 60 | 20 | 36 | 0.7 | 75 |
| 1340 | 5 | 35 | 0.45 | 55 | 10 | 37 | 0.4 | 60 | 15 | 38 | 0.41 | 65 | 20 | 40 | 0.3 | 80 |
|
|