BET surface area measurements obtained from SnO2 catalysts synthesized at temperatures of 400, 550, and 750°C [29].

content on SnO2 catalyst (wt.%)surface area (m2/g)
400°C550°C750°C

061.246.320.4
169.952.328.5
576.264.736.5
1590.280.857.2
20101.387.362.5
30129.5100.870.1