Calculated fiber content of CFRTP with 8 plies after resin removal by combustion according to ISO 14127.

OrganizationNumber of specimens Initial weight (g) Weight with wire (g) Weight after combustion (g) Fiber content in weight (%)
AverageStandard deviationAverageStandard deviationAverageStandard deviationAverageStandard deviation

A50.352740.014790.386920.018500.226740.0045754.6852.435
B50.353540.014290.384400.014550.228300.0057255.8861.243
C30.357430.005070.387930.003320.225930.0022254.6860.645
D30.357750.007910.609930.042290.460500.0540558.2083.702
E30.356260.004700.424980.001030.266430.0080155.5131.430
F50.356760.013310.379820.013770.226360.0021757.0662.264
G50.359880.008870.399060.008600.238040.0024755.2791.009
H50.361880.006110.418570.003630.253670.0038454.4400.578

Total340.357010.011150.415070.064670.256590.0668655.6472.194

Interlaboratory80.3570.0030.4240.0720.2660.07555.7201.227