Laboratory Performance Evaluation of HMA Modified with Various Types and Contents of Polymer
Table 4
Cyclic fatigue test summary.
Mix ID
Specimen ID
Test designation
Initial stress (kPa)-tension amplituded
Initial strain (microstrain)-peak to peakd
Frequency (Hz)
Cycle at failure
KS
KS-205
19a-CXb-Hc
1788
424
10
8,821
KS-202
19-CX-L
1552
247
10
69,008
K1
K1-205
19-CX-H
1717
391
10
10,856
K1-208
19-CX-L
1514
319
10
206,186
K2
K2-204
19-CX-H
1749
429
10
21,387
K2-206
19-CX-L
1658
307
10
224,764
K4
K4-202
19-CX-H
1950
308
10
2,731
K4-203
19-CX-L
1499
219
10
83,370