Index of flexural toughness and ductility of MSFRMM.

IDCuring timeASTM C1609
Flexural toughness, (kN·mm)Equivalent flexural strength ratio, (%)

S/C-0.67 d28.6976.5
S/C-0.824.8269.9
S/C-1.024.4770.0
W/C-0.167 d20.7070.7
W/C-0.1824.8269.9
W/C-0.2027.2777.8
MSF-0.4%12 h15.1663.8
MSF-0.8%21.2474.5
MSF-1.2%21.9272.6
MSF-1.6%21.6270.3
MSF-0.4%1 d18.7175.5
MSF-0.8%21.4573.2
MSF-1.2%24.2976.3
MSF-1.6%23.9666.1
MSF-0.4%3 d13.0162.6
MSF-0.8%24.3070.9
MSF-1.2%24.5170.8
MSF-1.6%25.5268.9
MSF-0.4%7 d18.0873.6
MSF-0.8%24.8269.9
MSF-1.2%26.0272.2
MSF-1.6%30.7165.7