Test results of the limestone samples in the conventional triaxial compression tests.
| Sample number | Confining pressure (MPa) | Loading rate (mm/s) | Strains at the peak stress point | Peak strength (MPa) | Average strength (MPa) | Axial | Circumferential | Volumetric |
| SA. 10 | 10.0 | 0.003 | 0.012177853 | −0.006236218 | −0.000294582 | 78.29 | 77.90 | SA. 11 | 10.0 | 0.003 | 0.011894353 | −0.006131956 | −0.000369558 | 74.49 | SA. 17 | 10.0 | 0.003 | 0.011926385 | −0.006141393 | −0.000356401 | 80.91 |
|
|