Research Article
A Model for the Analysis of Ultimate Capacity of RC and PC Corroded Beams
Table 2
Data of specimens tested by El Maaddawy et al. [
7].
| Code | Mass loss (%) | Bars’ attack penetration | Yield capacity | Ultimate capacity | Tensile (mm) | (mm) | (mm) | (kN) | (mm) | (kNm) | (kN) |
| Virgin | 0 | 0 | 67.2 | 15.6 | 75 | 73.3 | 37.5 | 37.5 | CN-50 | 8.9 | 0.7 | 61.7 | 14.4 | 70.2 | 89 | 35.1 | 35.1 | CN-110 | 14 | 1.1 | 57.4 | 13.9 | 66.8 | 78.4 | 33.4 | 33.4 | CN-210 | 22 | 1.8 | 50.7 | 13 | 60 | 62.4 | 30 | 30 | CN-310 | 31 | 2.7 | 44.1 | 11.7 | 53.3 | 59 | 31.2 | 31.2 | CS-50 | 9.7 | 0.8 | 59.9 | 12.3 | 66.1 | 73.4 | 33 | 33 | CS-110 | 15 | 1.2 | 55.1 | 8.9 | 64.6 | 85.9 | 32.3 | 32.3 | CS-210 | 22 | 1.9 | 50.1 | 8.4 | 64.2 | 79.9 | 32.1 | 32.1 | CS-310 | 30 | 2.6 | 46.1 | 7.4 | 56.9 | 66.8 | 28.4 | 28.4 |
|
|