The measuring results of experimental specimens.

SpecimenPu (kN)τu (MPa)Slip

C0-35-01169.319.17
C0-35-1501239.799.61
C0-35-10012610.0311.58
C0-45-01249.879.65
C0-45-15012610.0311.29
C0-45-10013510.7512.37
C0-55-015212.1013.65
C0-55-15015512.3414.05
C0-55-10016012.7418.19
C7-35-01078.526.79
C7-35-1501098.688.21
C7-35-1001159.168.93
C7-45-01219.637.62
C7-45-1501249.879.00
C7-45-10012710.1110.21
C7-55-012710.119.37
C7-55-15013810.9911.08
C7-55-10014811.7814.82
C15-35-0957.566.44
C15-35-150997.887.07
C15-35-1001007.968.28
C15-45-01007.967.27
C15-45-1501078.527.96
C15-45-1001149.089.86
C15-55-01249.878.17
C15-55-15012810.1910.45
C15-55-10014111.2313.80