Research Article
Design and Experimental Verification of Asphalt-Based Material for Grouting of Prestressed Structure
Table 1
Basic properties of AH70 asphalt and SBS asphalt.
| Content | AH70 asphalt | SBS asphalt | Test | Standard | Test | Standard |
| Penetration | 30°C 0.1 mm | 138.1 | | 90.3 | | 25°C 0.1 mm | 60.8 | 60–80 | 70.5 | >40 | 15°C 0.1 mm | 20.7 | | 28.3 | | Ductility (15°C) | cm | 174 | ≥100 | 153 | ≥100 | Softening point | °C | 52 | ≥46 | 63 | ≥60 | Wax content | % | 1.4 | <2.2 | 0.8 | <2.2 | Flash point | °C | 330 | ≥260 | 354 | ≥260 | Solubility | % | 99.7 | ≥99.5 | 99.9 | ≥99.5 | Density (15°C) | g/cm3 | 1.049 | | 1.026 | | Dynamic viscosity (60°C) | Pa·s | 220 | 160 | 183 | 160 | Flexible recovery (25°C) | % | 73 | >70 | 93 | >70 | RTFOT | Quality loss (%) | 0.37 | ≤±0.8 | 0.65 | <1 | Penetration ratio (%) | 72 | ≥61 | 92 | >65 | Ductility (cm) | 28.3 | ≥15 | 36.1 | >15 |
|
|