Research Article

Study on Fatigue Characteristics of Carbonation Erosion Prestressed Hollow Slabs in Whole Life Cycle

Table 11

The relation between deflections and strain and fatigue loading times for carbon-fiber-reinforced plate under the 200 kN load.

Fatigue times (104)Y-5 (με)Y-1 (με)W-1/2 (mm)

0208.8−290.31.06
50221.7−290.31.12
100237.6−307.11.29
150247.1−337.31.33
200260.3−362.31.44

Note. W-1/2: midspan deflection, Y-1: compressive strain at the top of the midspan, and Y-5: tension strain at the bottom of the midspan.