Mechanical Performance and Microstructure of Ultra-High-Performance Concrete Modified by Calcium Sulfoaluminate Cement

Table 2

Mixing design of UHPC.

ā€‰OPC (kg/m3)CSA (kg/m3)SF (kg/m3)GGBS (kg/m3)FA (kg/m3)Sand (kg/m3)SP (%)AA (%)

CSA0857.4053.653.6107.10.241071.70.6750.25
CSA5816.640.853.653.6107.10.241071.70.6750.25
CSA10779.477.953.653.6107.10.241071.70.6750.25
CSA15745.6111.853.653.6107.10.241071.70.6750.25
CSA20714.5142.953.653.6107.10.241071.70.6750.25

Note: : water-to-binder ratio; SP: superplasticizer; AA: antifoaming agent.