Study on Preparation of Coal Gangue-Based Geopolymer Concrete and Mechanical Properties

Table 4

Mixture ratio of coal gangue-based polymer concrete activated by dry powder (kg/m3).

NumbersCoal gangueFly ashSodium hydroxideCalcium carbonateSandPebbleWater-binder ratioPercentage of sand

G11961966611058312370.310.33
G21961966612062112480.330.33
G31961966614564012710.350.33
G41961964419857412160.380.32
G51961967219858812480.410.33
G61961969819865212930.430.34
G719619616861512530.300.33

1: water-binder ratio = quality of dry powder activator/(quality of dry powder activator + quality of coal gangue + quality of fly ash). 2: percentage of sand = quality of sand/(quality of sand + quality of pebble).