Results of energy spectrum analysis of collophane.

PointElement (%)
COFNaMgAlSiPCa

65874.9036.184.650.4414.2239.61
65884.0534.464.400.420.090.060.2514.3641.90
65893.8735.914.030.340.100.200.7613.0841.69
65904.8737.354.520.550.200.150.3713.6738.31
65914.0030.433.000.170.010.160.4215.9045.91
66013.7236.724.480.720.190.2513.6039.32
66023.2636.424.720.620.1613.5941.24
66032.3835.894.500.640.1013.8542.64
Average3.8835.424.290.490.110.070.2614.0341.33
Oxide content (%)Na2OMgOAl2O3SiO2P2O5CaO
0.660.180.130.5632.1557.83