Experimental Study on the Strength and Deformation Characteristics of Concrete under True Triaxial Compression after Sulfate Attack

Table 7

Uniaxial compressive strength and corrosion resistance coefficient of concrete specimens.

Time (d)Group WGroup SAverage strength of group W (MPa)Average strength of group S (MPa)K
123123

055.1458.1556.1555.1458.1556.1556.4856.481.00
3060.1463.5462.4162.1264.4263.2762.0363.271.02
6061.0465.6863.9659.7164.1363.0363.5662.290.98
9065.3666.2462.5862.3158.3460.0464.7660.230.93
12067.7966.6263.1152.8658.0956.9365.8455.960.85