Properties of SBS asphalt.

ItemTested resultRequirementTest method

Penetration (25°C, 100 g, 5 s) (0.1 mm)6860∼80T 0604
Penetration index0.32≥−0.4T 0604
Ductility (5°C, 5 cm/min) (cm)44≥30T 0605
Softening point (°C)77.9≥55T 0606
Kinematical viscosity (135°C) (Pa·s)1.73≤3T 0625
Flashpoint (°C)256≥230T 0611
Solubility in trichloroethylene (%)99.64≥99T 0607
Elastic recovery (%)85.8≥65T 0662
Density (25°C) (g/cm3)1.023T 0603
Storage stability (°C)1.3≤2.5T 0661
Thin film oven test (163°C)Mass loss (%)−0.04919−1.0–1.0T 0609
Residual penetration ratio (25°C) (%)73.5≥60T 0604
Residual ductility (5°C) (cm)26.37≥20T 0605