Research Article
A Method for Internal Curing Water Calculation of Concrete with Super Absorbent Polymer
Table 4
Results of air void characteristic in harden concrete.
| Samples | Air content (%) | Spacing factor (µm) | Air void distributions (%) | 0–200 µm | 200–1000 µm | 1000–4000 µm |
| A0 | 1.76 | 249 | 0.74 | 0.83 | 0.19 | A1 | 4.58 | 137 | 2.55 | 1.59 | 0.44 | A2 | 4.62 | 135 | 2.50 | 1.76 | 0.36 | B0 | 1.96 | 295 | 0.72 | 0.83 | 0.41 | B1 | 3.64 | 180 | 1.39 | 1.66 | 0.59 | B2 | 4.94 | 140 | 2.84 | 1.75 | 0.35 |
|
|