Fatigue test results at two stress levels.

SpecimenStress levelTest repetitionAverage SD
123

HMA40037,55637,57137,54837,55811.7
7005,4655,4605,4535,4596.0

LEA4007,5717,6097,5937,59119.1
7001,5371,5321,5261,5325.5

LEA + %10 CR40017,42917,45417,41917,43418.0
7003,3643,3533,3473,3558.6

LEA + %15 CR40019,73119,75519,74619,74412.1
7003,7493,7453,7633,7529.5

LEA + %15 CR40033,24833,24133,23733,2425.6
7004,9654,9824,9674,9719.3