Research Article
Effect of Nanoclay Filler on Fatigue Life of Natural Rubber/Styrene-Butadiene Blend
Table 3
Mechanical properties of different rubber samples.
| Row | Chemical material | Hardness (shore A) | Mean values of the tensile strength (MPa) | Standard deviation values | Mean values of tear strength (N/mm) | Standard deviation values |
| 1 | S70N30 | 44 | 6.78 | 0.86 | 11.23 | 0.96 | 2 | S50N50 | 47 | 7.21 | 2.03 | 14.54 | 0.67 | 3 | S40N60 | 49 | 7.82 | 0.58 | 19.07 | 1.14 | 4 | S50N50C5 | 49 | 7.66 | 0.73 | 15.78 | 0.31 | 5 | S40N60C3 | 51 | 9.73 | 0.62 | 16.87 | 0.17 | 6 | S40N60C5 | 53 | 10.81 | 0.40 | 21.72 | 1.59 | 7 | S40N60C7 | 52 | 10.24 | 1.25 | 20.16 | 2.11 |
|
|