Effect of the Composition of CAD/CAM Composite Blocks on Mechanical Properties

Table 2

Mean (SD) Vickers microhardness, nanohardness, elastic modulus, and the measured and manufacturers’ filler percentages by weight (wt%) for all tested materials. Values with the same superscript letters per column represent nonsignificant statistical difference for each individual property (α=0.05).

Material
type
Material
(code)
Microhardness
(Kg/mm2)
Nanohardness
(GPa)
Elastic Modulus
(GPa)
Manufacturers’ Filler
(wt)
measured filler
(wt)

Resin composite CAD/CAM blocksLava™- Ultimate (LU)112.6 (0.44)1.25 (0.05)12.14 (0.76)8074.8(0.1)
Shofu (SH)73.12 (1.04)0.775 (031)8.79 (0.35)6163 (0.02)
Cerasmart (CS)80.06 (0.76)0.81(0.006)10.36 (0.17)7066.1(0.2)
BRILLIANT
Crios (BC)
82.61(0.49)0.85 (0.008)10.98 (0.6)7170.1(0.05)
Grandio Blocs (GR)121.8(2.1)1.3(0.08)14.8(0.4)8684.6(0.01)

Polymer infiltrated ceramic network (PICN) ceramicVita Enamic
(EN)
203.1(0.43)3.1 (0.17)34.56 (1.4)8685.1(0.1)

Pure PEEKCeramill PEEK (PE)25.7 (0.05)0.317(0.008)2.53 (0.15)0.00(0)

Ceramic filled PEEKDentokeep (DK)27.74 (0.19)0.34(0.03)3.43 (0.29)2027.5(0.06)

Feldspathic ceramic blockVitablocs Mark II (VM)502.4 (2.28)6.83 (0.379)47.7 (3.47)100100(0)

EnamelEM313.3 (22.7)4.03(0.35)59.7(13)--

DentineDN62.3 (3.3)0.76( 0.13)16.5(2.3)--