Concentration of the “at risk” elements in each leachate from the batch reaction.

ElementAgCoGaMoSbSrVWTotal “at risk”
SamplePPBPPBPPBPPBPPBPPBPPBPPBPPB

HTLMix + DI water116.4151.30167.71
HTLMix + 0.1 M acetic acid77.2917.1520.4192.0467.67274.56
HTLMix + 0.1 M acetic acid 200°C26.484.001.04656.28141.60829.40
HTLMix + 0.013 M mineral acid3.762.6432.1084.800.24123.54
HTLMix + 0.13 M mineral acid 100°C159.0712.0017.483.49149.200.28341.52
HTLMix + 0.13 M mineral acid 200°C979.958.00176.007100.00220.007.988491.92
HTL315 + DI water1001.2871.931073.21
HTL315 + 0.1 M acetic acid1069.7590.0691.591251.40
HTL319 + DI water2.41181.83184.24
HTL319 + 0.1 M acetic acid128.04128.04
HTL321 + 0.013 M mineral acid11.642.6043.51101.20158.95
HTL324 + 0.013 M mineral acid5.520.440.1658.4064.52