Research Article
UAE Neem Extract as a Corrosion Inhibitor for Carbon Steel in HCl Solution
Table 6
The Effect of concentration of the aqueous extract of Neem leaves on surface coverage for carbon steel in 1.0 M HCl at various temperatures.
| | | Temperature/K | | | | | 303 | 313 | 323 | 333 | 343 | Concentration of Inhibitor | Surface Coverage | Surface Coverage | Surface Coverage | Surface Coverage | Surface Coverage |
| 1.0 M HCl + 0.02 g/L | 0.43 | 0.34 | 0.22 | 0.08 | −0.23 | 1.0 M HCl + 0.20 g/L | 0.65 | 0.57 | 0.36 | 0.10 | −0.18 | 1.0 M HCl + 0.50 g/L | 0.74 | 0.61 | 0.49 | 0.25 | −0.05 | 1.0 M HCl + 1.00 g/L | 0.77 | 0.63 | 0.56 | 0.35 | 0.04 | 1.0 M HCl + 2.00 g/L | 0.80 | 0.68 | 0.61 | 0.40 | 0.08 |
|
|