Effect of temperature on the corrosion parameters of zinc in 1.0 M HCl and 1.0 M HCl + 500 ppm of marjoram extract.
| System | (K) | (mV SCE) | (mA cm−2) |
IE (%) |
| 1.0 M HCl | 303 | −996 | 2.41 | — | 313 | −1002 | 2.81 | — | 323 | −1001 | 3.96 | — | 333 | −999 | 4.73 | — | 343 | −1001 | 5.58 | — |