Research Article

Study on the Electrochemical Performance of Sacrificial Anode Interfered by DC Stray Current

Table 3

The corrosion electrochemical parameters of the sacrificed anode interfered with different DC voltage.

Experiment days
(d)
DC
voltage
(V)
Cathodic slopeAnodic
slope
Polarization resistance (Ωcm2)Corrosion current density
(μA/mm2)

00-6.355.7725.1610.83
1-5.1314.8342.1842.31
3-5.1914.3862.6081.74
5-5.3924.6531.7812.43

20-4.7385.0275.7410.74
1-5.8134.3963.6701.63
3-4.729.5.4955.3631.59
5-5.0374.7012.0492.11

40-5.0925.1687.2060.43
1-4.6415.08214.6930.98
3-4.4475.3726.4520.66
5-5.6235.3722.1642.08

60-4.4385.1729.5610.43
1-4.7135.6265.7750.76
3-4.7324.9167.3540.52
5-5.1515.5172.4051.87

80-5.4055.8812.0631.55
1-4.7245.1186.3790.71
3-4.2514.9768.0180.49
5-4.2334.7773.6810.22