Specific surface area, pore volume, and pore radius of materials.

SampleSpecific surface area (m2/g)Pore volume (×10−3 cm3/g)Pore radius (Å)

MMT89.550.2308.7
Zr/MMT-590.021.9804.7
Zr/MMT-1097.501.9408.2
Zr/MMT-15128.662.3408.9

S-Zr/MMT-5213.940.4569.2
S-Zr/MMT-10265.450.3898.9
S-Zr/MMT-15287.110.3749.3
S-ZrO2225.080.7869.8