Research Article

A Nanomechanical Investigation of Three Putative Anti-Erosion Agents: Remineralisation and Protection against Demineralisation

Table 1

Mean nanohardness and standard deviations (GPa) of human enamel specimens as a function of stage and treatment. B: at baseline, D1: after first demineralisation, T: after treatment, D2: after second demineralisation.

TreatmentMean nanohardness (GPa) (Standard deviation)
BD1TD2

Negative control3.98 (0.37)2.58 (0.32)2.76 (0.35)2.29 (0.25)
1400 mg/L F4.25 (0.66)2.82 (0.32)3.28 (0.68)2.55 (0.28)
4500 mg/L F4.12 (0.52)2.56 (0.27)3.38 (0.54)2.82 (0.49)
CPP-ACP product4.30 (0.53)2.78 (0.36)3.22 (0.39)2.42 (0.27)
Positive control4.72 (0.46)2.86 (0.29)3.56 (0.50)3.06 (0.42)