Research Article
Effect of Glazing on Flexural Strength of Full-Contour Zirconia
Table 5
Flexural strength of highly translucent zirconia with different surface treatments.
| Zirconia | Flexural strength (MPa) ± standard deviation | Control | Heat-treated | Glazed |
| inCoris TZI | 970.17 ± 213.55 | 1148.86 ± 224.45 | 800.88 ± 117.12 | Prettau Zirconia | 1005.12 ± 180.85 | 1037.80 ± 82.81 | 815.00 ± 63.78 | Zirlux FC | 1017.36 ± 148.69 | 911.03 ± 127.67 | 853.62 ± 98.55 |
|
|