Research Article
The Corrosion Behaviour of WC-Co-Ru Alloys in Aggressive Chloride Media
Table 5
Electrochemical parameters for the samples in synthetic mine water.
| Sample (wt% Ru) | (V) | (A) ×10−6 | (V/Dec) | (V/Dec) | CR (mm/a) ×10−2 |
| 0.0 | −0.429 | 4.33 | 0.037 | 0.075 | 7.79 | 0.4 | −0.277 | 1.04 | 0.116 | 0.058 | 1.97 | 1.0 | −0.230 | 0.79 | 0.027 | 0.034 | 1.42 | 1.5 | −0.319 | 0.90 | 0.014 | 0.026 | 1.62 | 2.0 | −0.135 | 0.06 | 0.080 | 0.020 | 0.100 | 3.0 | −0.020 | 0.0002 | 0.040 | 0.018 | 0.004 | 0.4VC | −0.361 | 1.23 | 0.071 | 0.029 | 2.22 |
|
|