Growth of Anodic Aluminum Oxide Templates and the Application in Fabrication of the BiSbTe-Based Thermoelectric Nanowires

Table 1

Effects of deposition voltage on the composition of the -based materials; the deposition time was 60 min. Electrolyte formula was (a) 0.03 M Bi(NO3)3-5H2O and 0.04 M TeCl4 (b) 0.01 M Bi(NO3)3-5H2O, 0.01 M SbCl3, and 0.01 M TeCl4, respectively.

Compositions 0.03 M Bi(NO3)3-5H2O and 0.04 M TeCl4 0.01 M Bi(NO3)3-5H2O, 0.01 M SbCl3, and 0.01 M TeCl4

Potential (V)TeBiSbTeBi

0.0 V094.55.5
−0.2 V61.85538.155.3289.225.54
−0.3 V63.4836.5237.3544.0518.61
−0.4 V56.9443.0736.2344.0119.78
−0.5 V64.135.941.4233.7224.86
−0.6 V70.2329.7745.1544.7510.11