Research Article
Development of Back and Front Contacts for CdTe Layer in Tandem Flexible Photoelectric Converters on Basis of CdTe/CuInSe2
Table 3
Effect of annealing in air on the optical and electrical properties of ITO layers obtained at different substrate temperatures.
| (°C) | (μm) | (%) | (ohm/) | (ohm·cm) | (cm-3) | (cm2/(V·s)) |
| 20 | 0.51 | 71.5 | 41.4 | 21.1 | 1.0 | 29.6 | 200 | 0.50 | 72.2 | 38.3 | 19.1 | 1.1 | 29.7 | 250 | 0.54 | 71.8 | 31.1 | 16.8 | 1.2 | 31.0 | 300 | 0.49 | 72.3 | 23.7 | 11.6 | 1.7 | 31.7 | 350 | 0.52 | 71.1 | 18.5 | 9.6 | 1.9 | 34.3 | 400 | 0.53 | 70.9 | 15.5 | 8.2 | 2.2 | 34.6 | 430 | 0.54 | 72.0 | 11.1 | 6.0 | 2.8 | 37.2 |
|
|