Characteristic parameters of the cone calorimetric test for PP and flame retardant PP.

SamplesPHRRAV-HRRTHRAV-MLRResidue at 700 s
(kW/m2)(kW/m2)(MJ/m2)(g/s·m2) (wt%)

PP1128.7343.8149.50.0870
PP-1446.5229.3144.50.0558.3
PP-2775.0156.5130.90.0629.8
PP-6244.4208.9133.60.03623.8