Adding TiC Nanoparticles to Magnesium Alloy ZK60A for Strength/Ductility Enhancement

Table 3

Results of tensile testing of ZK60A and ZK60A/TiC nanocomposite.

Material0.2% TYS (MPa)UTS (MPa)Failure strain (%)WOF (MJ/m3)a

ZK60A163 ± 3268 ± 36.6 ± 0.616 ± 2
ZK60A/1.5 vol.% TiC184 ± 2 (+13)309 ± 3 (+15)11.6 ± 1.4 (+76)33 ± 5 (+106)

aObtained from engineering stress-strain diagram using EXCEL software.
( ) Brackets indicate % change with respect to corresponding result of ZK60A.