Research Article
Nanowires of Lead-Free Solder Alloy SnCuAg
Table 1
Bath contents and electrodeposition conditions for production of SnCuAg nanowires.
| Chemicals | Concentration |
| SnCl2 · 2H2O | 40 mM | CuCl2 · 2H20 | 1 mM | Ag(NO3)2 | 5 mM | C6H17N3O7 | 95 mM |
| Operating conditions | |
|
Bath pH 4 |
Bath temperature = room temperature |
Deposition duration = 180 min |
Deposition potential = −0.75 V–−2 V, versus Ag/AgCl |
Agitation paddle (5 cycles/s) |
|
|