Research Article

Functionalization of Mesoporous Silicon Nanoparticles for Targeting and Bioimaging Purposes

Table 1

The hydrodynamic size, polydispersity index (PDI), and zeta-potential of the UnTHCPSi nanoparticles with different PEGylations. O-PEG is adsorbed to UnTHCPSi-NP surface while C-PEG is covalently bound with amide linkage.

UnTHCPSi-NP PEGylationHydrodynamic size (nm)PDIZeta-potential (mV)

none139.6 ± 0.70.082 ± 0.011−31.7 ± 0.4
O-PEG 5k Da137.6 ± 1.20.093 ± 0.006−28.7 ± 0.1
O-PEG 10 kDa145.3 ± 1.20.089 ± 0.006−26.6 ± 0.8
O-PEG 20 kDa146.9 ± 1.60.079 ± 0.017−25.6 ± 0.3
C-PEG 5 kDa134.5 ± 1.00.111 ± 0.004−35.5 ± 0.2
C-PEG 10 kDa146.6 ± 0.60.081 ± 0.024−32.7 ± 0.7
C-PEG 20 kDa152.8 ± 1.50.109 ± 0.036−29.0 ± 0.5

The values are represented as an average of three measurements ± standard deviation.