Research Article
Simple Method for the Preparation of Composites Based on PA6 and Partially Exfoliated Graphite
Table 2
Results of mechanical tests.
| | Modulus (Mpa) | Strain at break (%) | Max yield stress (Mpa) | Stress at break (Mpa) |
| PA6 | 3275 | 0.7 | ā | 17 | PA6(0.5) | 1820 | 1.2 | ā | 20 | PA6(1.0) | 2087 | 26.0 | 16 | 11 |
|
|