Research Article

Effect of Nanometric Metallic Hydroxides on the Flame Retardant Properties of HDPE Composites

Table 5

Data obtained from the cone calorimeter: time to ignition, time to reach the PHRR, heat release rate at the peak (PHRR), total heat released (THR) since ignition to flameout, and time to flameout.

Time to ignition [s]Time to peak HRR [s]Peak HRR [(kJ/s)/m²]THR [MJ/m²]Time to flameout [s]

HDPE631502030.11110.58178

M386155255.3586.71593
A365125257.7593.64710
MA367120265.2999.91709
MA3maleic76125240.4479.61597
MA3acryl80125256.6387.53681

Note: 1 W = 1 J/s.
Data for HDPE was also obtained experimentally, though it is not shown in Figure 3.