Gold Nanoparticles Size Design and Control by Poly(N,N′-diethylaminoethyl methacrylate)
Table 1
Synthesis results of AuNPs prepared at different reaction conditions.
Reaction (RX)
Polymer
in g/mol ()
Solvent
pH
Ratio polymer : Au (mg/mg)
(nm)
(nm)
(nm)
1
None
—
Water
7
4 : 1
543
19
—
2
PDEAEM
9000 (1.18)
Water
4.8
3.75 : 1
520
110
4.9 ± 0.9
3
PDEAEM
18000 (1.97)
Water
4.8
3.75 : 1
520
13
7.5 ± 0.8
4
PDEAEM
24500 (1.31)
Water
4.8
3.75 : 1
521
19
4.4 ± 1.4
5
PDEAEM
29300 (1.1)
Water
4
4 : 1
519
21
4.4 ± 0.9
6
PDEAEM
18000 (1.97)
Water
3
3.75 : 1
526
27
15 ± 1.8
7
PDEAEM
29300 (1.1)
Dioxane : water (15 : 1)
—
4 : 1
526
—
10.1 ± 1.1
8
PDEAEM
18000 (1.97)
Ethanol
—
3.75 : 1
521
72
4.6 ± 1.5
9
PDEAEM
18000 (1.97)
Isopropanol
—
3.75 : 1
531
569
3.5 ± 1.0
is the number average molecular weight; = / is the dispersity in molecular weight. is the maximum of the surface plasmon resonance peak. is the hydrodynamic diameter of AuNPs@PDEAEM. is the average diameter of AuNPs by scanning transmission electron microscopy (STEM).