Research Article
Silica Based Superhydrophobic Nanocoatings for Natural Rubber Surfaces
Table 1
Mechanical properties of the coated natural rubber surfaces.
| Property | Sample | Control | Dipped coated | Spray coated |
| Cure time (hours) | 24 | 24 | 24 | Cure temperature (°C) | 50 | 50 | 50 | Tensile strength (MPa) | 16.22 ± 6.09 | 11.58 ± 2.24 | 15.65 ± 1.35 | Mod 100% (MPa) | 1.40 ± 0.13 | 1.36 ± 0.08 | 1.44 ± 0.25 | Mod 500% (MPa) | 8.35 ± 1.54 | 7.43 ± 2.44 | 8.58 ± 1.55 | Tear strength (kN/m) | 43.48 ± 5.66 | 29.39 ± 1.90 | 30.52 ± 2.38 |
|
|