Sample type-test 1, strain range 0.3–0.6 []-test 2, strain range 0.3–0.6 []-test 3, strain range 0.3–0.6 []-test 3, strain range 1.0–1.3 []Maximum current increase at the breaking point []Maximum strain []Strength MPa]

Neat epoxy8.659.4
Sample 80.7 ± 0.10.5 ± 0.20.7 ± 0.12.1 ± 0.32.7 ± 0.62.0 ± 0.238.9 ± 1.9
Sample 90.3 ± 0.10.3 ± 0.10.3 ± 0.11.3 ± 0.22.0 ± 0.11.7 ± 0.442.0 ± 0.2
Sample 100.4 ± 0.10.6 ± 0.50.7 ± 0.51.2 ± 0.12.3 ± 0.61.9 ± 0.138.5 ± 3.3
Sample 110.8 ± 0.70.6 ± 0.10.7 ± 0.11.6 ± 0.12.3 ± 0.61.7 ± 0.337.8 ± 1.0