Thicknesses and yields of electrodepositions for three concentrations of Ce3+ ions.

Deposition time (h)Concentration of Ce3+ ions (mg/mL)
0.0460.0922.0
Thickness (mg/cm2)Yield (%)Thickness (mg/cm2)Yield (%)Thickness (mg/cm2)Yield (%)

0.50.015 ± 0.01424 ± 220.021 ± 0.01517 ± 120.16 ± 0.025.7 ± 0.9
20.057 ± 0.01091 ± 160.050 ± 0.01440 ± 110.40 ± 0.0415 ± 1
40.067 ± 0.015106 ± 250.090 ± 0.01972 ± 150.43 ± 0.0316 ± 1
60.054 ± 0.02286 ± 350.099 ± 0.01878 ± 150.42 ± 0.0315 ± 1
80.067 ± 0.062106 ± 400.150 ± 0.036120 ± 290.35 ± 0.0313 ± 1