Research Article
Elastomeric Nanocomposite Based on Exfoliated Graphene Oxide and Its Characteristics without Vulcanization
Table 4
Tensile properties of unvulcanized GO/NBR nanocomposites at different GO loadings.
| GO loading wt% (g) | Tensile stress at max. load (MPa) | Tensile strain at max. load % | Modulus at max. load (MPa) | Tensile extension at max. load (mm) | Modulus at elastic region (MPa) |
| 0.0 | 0.32 | 1088.66 | 0.342 | 435.46 | 0.423 | 0.2 | 0.29 | 476.58 | 0.223 | 190.63 | 1.042 | 0.4 | 0.44 | 842.56 | 0.271 | 337.02 | 1.042 | 0.8 | 0.50 | 705.11 | 0.365 | 282.04 | 1.403 | 1.0 | 0.58 | 573.92 | 0.382 | 229.56 | 1.430 |
|
|