Research Article

Experimental Analysis on Tribological Characteristics of AZ60A/Gr/BN Magnesium Composites

Table 3

Design of experiments using L27 (orthogonal array).

Ex. no.Composite weight (%)Speed at slidingLoadWear rateSignal-to-noise ratio

111.045300.004647.526
211.045600.004847.541
311.045900.005046.201
411.59300.005246.105
511.59900.005646.182
611.59600.012838.104
712.08300.005945.201
812.08900.006145.124
912.08600.012439.221
1021.045300.004248.801
1121.045900.004648.231
1221.045600.004947.526
1321.59300.005047.424
1421.59900.005246.952
1521.59600.012039.466
1622.08300.005646.281
1722.08900.005945.981
1822.08600.011939.441
1931.045300.004149.364
2031.045900.003948.286
2131.045600.004148.206
2231.59300.004148.206
2331.59900.004547.441
2431.59600.005146.526
2532.08300.005146.526
2632.08900.005246.321
2732.08600.005945.312