Optimization on Stir Casting Process Parameters of Al7050/Nano-B4C Metal Matrix Composites

Table 4

L9 stir casting process parameters with microhardness.

Ex. nowt% B4C (A)Melting temperature (°C) (B)Stirring speed (rpm) (C)Stirring time (min) (D)Microhardness

1370030010162
2375035015171.5
3380040020164
4670035020173
5675040010175.5
6680030015175
7970040015182
8975030020185
9980035010185.5