Research Article

Preparation and Sealing Processing of Sodium Alginate Based Blending Film

Table 1

Film sealing experiment design with coded and real values for adhesive concentration, sealing temperature, and sealing pressure along with response variable of seal strength.

Trial numberIndependent variablesResponse variable
Coded valuesReal values
Adhesive concentration
(%)
Sealing temperature
(°C)
Sealing pressure
(MPa)
Seal strength
(N/15 mm)

1111261550.3521.33
211−1261550.2524.66
31−11261450.3523.13
41−1−1261450.2519.23
5−111221550.3520.13
6−11−1221550.2524.09
7−1−11221450.3518.16
8−1−1−1221450.2520.17
91.6820027.3641500.319.81
101.6820020.6361500.316.50
1101.682024158.410.323.04
1201.682024141.590.321.67
13001.682241500.38420.63
14001.682241500.21623.36
15000241500.325.35
16000241500.324.93
17000241500.325.56
18000241500.324.20
19000241500.324.82
20000241500.324.20