No.Particle size S (A)Grinding speed Wt (B)Setting cut depth Ap (C)Feed rate Vf (D)Surface roughness (Ra)SNR

1.32045000.10.50.03728.64

2.32045000.210.07422.62

3.32045000.320.08821.11

4.32060000.30.50.06923.22

5.32075000.320.03030.46

6.60045000.110.07922.05

7.60045000.220.05924.58

8.60075000.310.07222.85

9.60045000.220.05525.19

10.60045000.30.50.10819.33

11.60060000.120.11718.64

12.60060000.20.50.14516.77

13.60075000.210.13917.14

14.60075000.320.10619.49

15.100045000.20.50.03728.64

16.100045000.320.04726.56

17.100045000.10.50.07222.85

18.100045000.210.04626.74

19.100075000.210.03529.12

20.100075000.110.04526.94

21.100075000.220.11119.09

22.100075000.30.50.10519.58

23.32075000.20.50.29410.63

24.60045000.110.08321.62

25.60060000.310.09420.54

26.60075000.10.50.07422.62

27.100045000.120.10719.41

28.60060000.110.11518.79

29.60045000.310.08221.72

30.32045000.310.06423.88